BS EN 10217-7 2005 is the material standard for stainless steels for welded tubes for pressure purposes. This new standard was first published in February 2005.
As an alternative to scanning down the list try the ‘find’ facility on your keyboard, using the ‘Ctrl’ and ‘F’ keys together. Type in the term you are looking for in the dialog box that then appears.
The data given is not intended to replace that shown in individual standards to which reference should always be made.
Tensile properties at RT | Impact properties | ||||||||||||
Steel grade | Proof Strength | Tensile strength | Elongation | Minimum average of 3 Charpy (J) | |||||||||
Rp0.2 | Rp1.0 | Rm | A min (%) | at RT | at -sub-zero temperature1 | ||||||||
Steel name | Steel number | MPa | MPa | MPa | long | trans | long | trans | trans | ||||
Austenitic steels | |||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|
X2CrNi18-9 | 1.4307 | 180 | 215 | 470-670 | 40 | 35 | 100 | 60 | 60 | ||||
X2CrNi19-11 | 1.4306 | 180 | 215 | 460-680 | 40 | 35 | 100 | 60 | 60 | ||||
X2CrNiN18-10 | 1.4311 | 270 | 305 | 550-760 | 35 | 30 | 100 | 60 | 60 | ||||
X5CrNi18-10 | 1.4301 | 195 | 230 | 500-700 | 40 | 35 | 100 | 60 | 60 | ||||
X6CrNiTi18-10 | 1.4541 | 200 | 235 | 500-730 | 35 | 30 | 100 | 60 | 60 | ||||
X6CrNiNb18-10 | 1.4550 | 205 | 240 | 510-740 | 35 | 30 | 100 | 60 | 60 | ||||
X2CrNiMo17-12-2 | 1.4404 | 190 | 225 | 490-690 | 40 | 30 | 100 | 60 | 60 | ||||
X5CrNiMo17-12-2 | 1.4401 | 205 | 240 | 510-710 | 40 | 30 | 100 | 60 | 60 | ||||
XCrNiMoTi17-12-2 | 1.4571 | 210 | 245 | 500-730 | 35 | 30 | 100 | 60 | 60 | ||||
X2CrNiMo17-12-3 | 1.4432 | 190 | 225 | 490-690 | 40 | 30 | 100 | 60 | 60 | ||||
X2CrNiMoN17-13-3 | 1.4429 | 295 | 330 | 580-800 | 35 | 30 | 100 | 60 | 60 | ||||
X3CrNiMo17-13-3 | 1.4436 | 205 | 240 | 510-710 | 40 | 30 | 100 | 60 | 60 | ||||
X2CrNiMo18-14-3 | 1.4435 | 190 | 225 | 490-690 | 40 | 30 | 100 | 60 | 60 | ||||
X2CrNiMoN17-13-5 | 1.4439 | 285 | 315 | 580-800 | 35 | 30 | 100 | 60 | 60 | ||||
X2CrNiMo18-15-4 | 1.4438 | 220 | 250 | 490-690 | 35 | 30 | 100 | 60 | 60 | ||||
X1NiCrMoCu31-27-4 | 1.4563 | 215 | 245 | 500-750 | 40 | 35 | 120 | 90 | 60 | ||||
X1CrNiMoCu25-20-5 | 1.4539 | 220 | 250 | 520-720 | 35 | 30 | 120 | 90 | 60 | ||||
X1CrNiMoCuN20-18-7 | 1.4547 | 300 | 340 | 650-850 | 35 | 30 | 100 | 60 | 60 | ||||
X1NiCrMoCuN25-20-7 | 1.4529 | 300 | 340 | 600-800 | 40 | 40 | 120 | 90 | 60 | ||||
Duplex – Austenitic ferritic steels | |||||||||||||
X2CrNiN23-4 | 1.4362 | 400 | —- | 600-820 | 25 | 25 | 120 | 90 | 40 | ||||
X2CrNiMoN22-5-3 | 1.4462 | 450 | —- | 700-920 | 25 | 20 | 120 | 90 | 40 | ||||
X2CrNiMoN25-7-4 | 1.4410 | 550 | —- | 800-1000 | 20 | 20 | 100 | 100 | 40 | ||||
X2CrNiMoCuWN25-7-4 | 1.4501 | 550 | —- | 800-1000 | 20 | 20 | 100 | 100 | 40 |
1.For austenitic steels the sub-zero test temperature is -196 deg C. For duplex steels it is – 40 deg C.
Steel grade | Rp0.2 min MPa at a temperature of (deg C) | |||||||||||
Steel name | Steel number | 50 | 100 | 150 | 200 | 250 | 300 | 350 | 400 | 450 | 500 | 550 |
X2CrNi18-9 | 1.4307 | 165 | 147 | 132 | 118 | 108 | 100 | 94 | 89 | 85 | 81 | 80 |
X2CrNi19-11 | 1.4306 | 165 | 147 | 132 | 118 | 108 | 100 | 94 | 89 | 85 | 81 | 80 |
X2CrNiN18-10 | 1.4311 | 255 | 205 | 175 | 157 | 145 | 136 | 130 | 125 | 121 | 119 | 118 |
X5CrNi18-10 | 1.4301 | 180 | 157 | 142 | 127 | 118 | 110 | 104 | 98 | 95 | 92 | 90 |
X6CrNiTi18-10 | 1.4541 | 190 | 176 | 167 | 157 | 147 | 136 | 130 | 125 | 121 | 119 | 118 |
X6CrNiNb18-10 | 1.4550 | 195 | 177 | 167 | 157 | 147 | 136 | 130 | 125 | 121 | 119 | 118 |
X2CrNiMo17-12-2 | 1.4404 | 182 | 166 | 152 | 137 | 127 | 118 | 113 | 108 | 103 | 100 | 98 |
X5CrNiMo17-12-2 | 1.4401 | 193 | 177 | 162 | 147 | 137 | 127 | 120 | 115 | 112 | 110 | 108 |
XCrNiMoTi17-12-2 | 1.4571 | 202 | 185 | 177 | 167 | 157 | 145 | 140 | 135 | 131 | 129 | 127 |
X2CrNiMo17-12-3 | 1.4432 | 182 | 166 | 152 | 137 | 127 | 118 | 113 | 108 | 103 | 100 | 98 |
X2CrNiMoN17-13-3 | 1.4429 | 260 | 211 | 185 | 167 | 155 | 145 | 140 | 135 | 131 | 129 | 127 |
X3CrNiMo17-13-3 | 1.4436 | 195 | 177 | 162 | 147 | 137 | 127 | 120 | 115 | 112 | 110 | 108 |
X2CrNiMo18-14-3 | 1.4435 | 180 | 165 | 150 | 137 | 127 | 119 | 113 | 108 | 103 | 100 | 98 |
X2CrNiMoN17-13-5 | 1.4439 | 260 | 225 | 200 | 185 | 175 | 165 | 155 | 150 | — | — | — |
X2CrNiMo18-15-4 | 1.4438 | 200 | 172 | 157 | 147 | 137 | 127 | 120 | 115 | 112 | 110 | 108 |
X1NiCrMoCu31-27-4 | 1.4563 | 210 | 190 | 175 | 160 | 155 | 150 | 145 | 135 | 125 | 120 | 115 |
X1CrNiMoCu25-20-5 | 1.4539 | 216 | 205 | 190 | 175 | 160 | 145 | 135 | 125 | 115 | 110 | 105 |
X1CrNiMoCuN20-18-7 | 1.4547 | 267 | 230 | 205 | 190 | 180 | 170 | 165 | 160 | 153 | 148 | — |
X2CrNiMoCuWN25-7-4 | 1.4529 | 270 | 230 | 210 | 190 | 180 | 170 | 165 | 160 | 130 | 120 | 105 |
Steel grade | Rp1.0 min MPa at a temperature of (deg C) | |||||||||||
Steel name | Steel number | 50 | 100 | 150 | 200 | 250 | 300 | 350 | 400 | 450 | 500 | 550 |
X2CrNi18-9 | 1.4307 | 200 | 181 | 162 | 147 | 137 | 127 | 121 | 116 | 112 | 109 | 108 |
X2CrNi19-11 | 1.4306 | 200 | 181 | 162 | 147 | 137 | 127 | 121 | 116 | 112 | 109 | 108 |
X2CrNiN18-10 | 1.4311 | 282 | 240 | 210 | 187 | 175 | 167 | 161 | 156 | 152 | 149 | 147 |
X5CrNi18-10 | 1.4301 | 218 | 191 | 172 | 157 | 145 | 135 | 129 | 125 | 122 | 120 | 120 |
X6CrNiTi18-10 | 1.4541 | 222 | 208 | 196 | 186 | 177 | 167 | 161 | 156 | 152 | 149 | 147 |
X6CrNiNb18-10 | 1.4550 | 232 | 211 | 196 | 186 | 177 | 167 | 161 | 156 | 152 | 149 | 147 |
X2CrNiMo17-12-2 | 1.4404 | 217 | 199 | 181 | 167 | 157 | 145 | 139 | 135 | 130 | 128 | 127 |
X5CrNiMo17-12-2 | 1.4401 | 230 | 211 | 191 | 177 | 167 | 156 | 150 | 144 | 141 | 139 | 137 |
XCrNiMoTi17-12-2 | 1.4571 | 232 | 218 | 206 | 196 | 186 | 175 | 169 | 164 | 160 | 158 | 157 |
X2CrNiMo17-12-3 | 1.4432 | 217 | 199 | 181 | 167 | 157 | 145 | 139 | 135 | 130 | 128 | 127 |
X2CrNiMoN17-13-3 | 1.4429 | 290 | 246 | 218 | 198 | 183 | 175 | 169 | 164 | 160 | 158 | 157 |
X3CrNiMo17-13-3 | 1.4436 | 228 | 211 | 191 | 177 | 167 | 156 | 150 | 144 | 141 | 139 | 137 |
X2CrNiMo18-14-3 | 1.4435 | 217 | 200 | 180 | 165 | 153 | 145 | 139 | 135 | 130 | 128 | 127 |
X2CrNiMoN17-13-5 | 1.4439 | 290 | 255 | 230 | 210 | 200 | 190 | 180 | 175 | — | — | — |
X2CrNiMo18-15-4 | 1.4438 | 232 | 206 | 188 | 177 | 167 | 156 | 148 | 144 | 140 | 138 | 136 |
X1NiCrMoCu31-27-4 | 1.4563 | 240 | 220 | 205 | 190 | 185 | 180 | 175 | 165 | 155 | 150 | 145 |
X1CrNiMoCu25-20-5 | 1.4539 | 244 | 235 | 220 | 205 | 190 | 175 | 165 | 155 | 145 | 140 | 135 |
X1CrNiMoCuN20-18-7 | 1.4547 | 306 | 270 | 245 | 225 | 212 | 200 | 195 | 190 | 184 | 180 | — |
X2CrNiMoCuWN25-7-4 | 1.4529 | 310 | 270 | 245 | 225 | 215 | 205 | 195 | 190 | 160 | 150 | 135 |