BS EN 10269 is the material standard for stainless and heat-resisting steels, a selection of low alloy steels and some nickel alloys for fasteners. The standard includes some elevated and sub-zero temperature mechanical properties and can be used for specifying fasteners for pressure purposes. Austenitic, martensitic and precipitation hardening stainless grades are included. Only the chemical composition of the stainless steels in the standard are listed in this article.
As an alternative to scanning down the list try the ‘find’ facility on your keyboard, using the ‘Ctrl’ and ‘F’ keys together. Type in the term you are looking for in the dialog box that then appears.
The data given is not intended to replace that shown in individual standards to which reference should always be made.
Designation | Chemical composition (% by mass – max unless stated) | ||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|
Steel name | Steel number | C | Si | Mn | P max | S max | Al tot | B | Cr | Mo | Ni | V | Others |
Steels for quenching and tempering | |||||||||||||
X22CrMoV12-1 | 1.4923 | 0.18/0.24 | 0.50 | 0.40/0.90 | 0.025 | 0.015 | – | – | 11.00/12.50 | 0.80/1.20 | 0.30/0.80 | 0.20/0.35 | – |
X12CrNiMoV12-3 | 1.4938 | 0.08/0.15 | 0.50 | 0.40/0.90 | 0.025 | 0.015 | – | – | 11.00/12.50 | 1.50/2.00 | 2.00/3.00 | 0.25/0.40 | N 0.020/0.040 |
X19CrMoNbVN11-1 | 1.4913 | 0.17/0.23 | 0.50 | 0.40/0.90 | 0.025 | 0.015 | 0.020 | 0.0015 | 10.00/11.50 | 0.50/0.80 | 0.20/0.60 | 0.10/0.30 | N 0.25/0.55: N 0.05/0.10 |
Austenitic steels | |||||||||||||
X2CrNi18-9 | 1.4307 | 0.030 | 1.00 | 2.00 | 0.045 | 0.030 | – | – | 17.50/19.50 | – | 8.00/10.00 | – | N 0.11 |
X5CrNi18-10 | 1.4301 | 0.07 | 1.00 | 2.00 | 0.045 | 0.030 | – | – | 17.00/19.50 | – | 8.00/10.50 | – | N 0.11 |
X4CrNi18-12 | 1.4303 | 0.06 | 1.00 | 2.00 | 0.045 | 0.030 | – | – | 17.00/19.00 | – | 11.00/13.00 | – | N 0.11 |
X2CrNiMo17-12-2 | 1.4404 | 0.030 | 1.00 | 2.00 | 0.045 | 0.030 | – | – | 16.50/18.50 | 2.00/2.50 | 10.00/13.00 | – | N 0.11 |
X5CrNiMo17-12-2 | 1.4401 | 0.07 | 1.00 | 2.00 | 0.045 | 0.030 | – | – | 16.50/18.50 | 2.00/2.50 | 10.00/13.00 | – | N 0.11 |
X2CrNiMoN17-13-3 | 1.4429 | 0.030 | 1.00 | 2.00 | 0.045 | 0.030 | – | – | 16.50/18.50 | 2.50/3.00 | 11.00/14.00 | – | N 0.12/0.22 |
X3CrNiCu18-9-4 | 1.4567 | 0.04 | 1.00 | 2.00 | 0.045 | 0.030 | – | – | 17.00/19.00 | – | 8.50/10.50 | – | N 0.11: Cu 3.00/4.00 |
X6CrNi18-10 | 1.4948 | 0.04/0.08 | 1.00 | 2.00 | 0.035 | 0.015 | – | – | 17.00/19.00 | – | 8.00/11.00 | – | N 0.11 |
X10CrNiMoMnNbVB15-10-1 | 1.4982 | 0.07/0.13 | 1.00 | 5.50/7.00 | 0.040 | 0.030 | – | 0.003/0.009 | 14.00/16.00 | 0.80/1.20 | 9.00/11.00 | 0.15/0.40 | N 0.11: Nb 0.75/1.25 |
X3CrNiMoBN17-13-3 | 1.4910 | 0.04 | 0.75 | 2.00 | 0.035 | 0.015 | – | 0.0015/0.0050 | 16.00/18.00 | 2.00/3.00 | 12.00/14.00 | – | N 0.10/0.18 |
X6CrNiMoB17-12-2 | 1.4919 | 0.04/0.08 | 1.00 | 2.00 | 0.035 | 0.015 | – | 0.0015/0.0050 | 16.50/18.50 | 2.00/2.50 | 10.00/13.00 | – | N 0.11 |
X6CrNiTiB18-10 | 1.4941 | 0.04/0.08 | 1.00 | 2.00 | 0.035 | 0.015 | – | 0.0015/0.0050 | 17.00/19.00 | – | 9.00/12.00 | – | Ti 5 x C/0.80 |
X6NiCrTiMoVB25-15-2 | 1.4980 | 0.03/0.08 | 1.00 | 1.00/2.00 | 0.025 | 0.015 | 0.35 | 0.0030/0.010 | 13.50/16.00 | 1.00/1.50 | 24.00/27.00 | 0.10/0.50 | Ti 1.90/2.30 |
X7CrNiMoBNb16-16 | 1.4986 | 0.04/0.10 | 0.30/0.60 | 1.00 | 0.045 | 0.030 | – | 0.05/0.10 | 15.50/17.50 | 1.60/2.00 | 15.50/17.50 | – | Nb+Ta 10xC/1.20 |
Note
Al tot – total aluminium