Ambient temperature mechanical properties of ferritic stainless steel flat products to BS EN 10088-2

Introduction

BS EN 10088-2 is the material standard for stainless steel sheet, plate and strip for general purposes. This article gives the 0.2% and 1.0% proof strength, tensile strength and elongation of the 26 ferritic grades specified. The standard also specifies the resistance to intergranular corrosion acceptance criteria. For reasons of space, these are omitted from the tables shown here.

As an alternative to scanning down the list try the ‘find’ facility on your keyboard, using the ‘Ctrl’ and ‘F’ keys together. Type in the term you are looking for in the dialog box that then appears.

The data given is not intended to replace that shown in individual standards to which reference should always be made.

BS EN 10088-2:2005 Edition

BS EN 10088-2 was originally published in 1995. The second version BS EN 10088-2:2005 has been superseded by BS EN 10088-2:2014.

The tables shown here only have the 2014 tensile property ranges of the ferritic steels. Six new ferritic grades 1.4600, 1.4607, 1.4611, 1.4613, 1.4630 and 1.4634 have been added.

BS EN 10088-2 mechanical properties – ferritic stainless steels

Designation Mechanical properties min unless stated
Steel name Steel number Product Proof strength Rp0.2 N/mm2 Tensile strength Rm N/mm2 Elongation A80mm2) for < 3mm A3) for > 3mm
Form1) Max thickness mm Longitudinal Transverse %
Ferritic stainless steels at room temperatures in the annealed condition- standard grades
X2CrNi12 1.4003 C 8 280 320 450/650 20
H 13.5 280 320 450/650 20
P 254) 250 280 450/650 18
X2CrTi12 1.4512 C 8 210 220 380/560 25
H 13.5 210 220 380/560 25
X6CrNiTi12 1.4516 C 8 280 320 450/650 23
H 13.5 280 320 450/650 23
P 254) 250 280 450/650 20
X6Cr13 1.4000 C 8 240 250 400/600 19
H 13.5 220 230 400/600 19
P 254) 220 230 400/600 19
X6CrAl13 1.4002 C 8 230 250 400/600 17
H 13.5 210 230 400/600 17
P 254) 210 230 400/600 17
X6Cr17 1.4016 C 8 260 280 450/600 20
H 13.5 240 260 450/600 18
P 254) 240 260 430/630 20
X3CrTi17 1.4510 C 8 230 240 420/600 23
H 13.5 230 240 420/600 23
X3CrNb17 1.4511 C 8 230 240 420/600 23
X6CrMo17-1 1.4113 C 8 260 280 450/630 18
H 13.5 260 280 450/630 18
X2CrMoTi18-2 1.4521 C 8 300 320 420/640 20
H 13.5 280 300 400/600 20
P 12 280 300 420/620 20
Ferritic stainless steels at room temperatures in the annealed condition- special grades
X2CrMnNiTi12 1.4600 H 10 375 500/650 20
X2CrSiTi15 1.4630 C 8 210 230 380/580 20
X2CrTi17 1.4520 C 8 180 200 380/530 24
X1CrNb15 1.4595 C 8 210 220 380/560 25
X2CrMoTi17-1 1.4513 C 8 200 220 400/550 23
X6CrNi17-1 1.4017 C 8 330 350 500/750 12
X5CrNiMoTi15-2 1.4589 C 8 400 420 550/750 16
H 13.5 360 380 550/750 14
X6CrMoNb17-1 1.4526 C 8 280 300 480/560 25
X2CrNbZr17 1.4590 C 8 230 250 400/550 23
X2CrTiNb18 1.4509 C 8 230 250 430/630 18
X2CrAlSiNb18 1.4634 C 8 240 260 430/650 18
X2CrNbTi20 1.4607 C 8 230 250 430/630 18
X2CrTi21 1.4611 C 8 230 250 430/630 18
X2CrTi24 1.4613 C 8 230 250 430/630 18
X2CrMoTi29-4 1.4592 C 8 430 450 550/700 20

Note

  1. C= Cold rolled strip; H= hot rolled strip; P= hot rolled plate.
  2. The values apply for test pieces with a gauge length of 80mm and a width of 20mm. Test pieces with a gauge length of 50mm and a width of 12.5mm can also be used.
  3. The values apply for test pieces with a gauge length of 5.65 So0.5
  4. For thicknesses above 25mm, the mechanical properties can be agreed.

 