Ambient temperature mechanical properties for BS EN 10253-3 and 10253-4 for stainless steel butt weld fittings
Introduction
BS EN 10253-3 is the material standard for austenitic and duplex stainless steels for butt-welded fittings without specific inspection requirements.
BS EN 10253-4 is the material standard for austenitic and duplex stainless steels for butt-welded fittings with specific inspection requirements.
The compositions are the same in both standards. They differ in that part 4 has a comprehensive set of inspection requirements. The overall intention seems to be that part 4 makes the fittings suitable for pressure purposes. The extra requirements of part 4 include;
- Definition of product making process – starting forms, hot and cold processing
- Normal or enhanced wall thickness
- Impact toughness values
- Determination of pressure factors – formulae are given for calculating these and tables are provided for common fitting sizes
The types of product covered by the standards are:
- Elbows
- Concentric reducers
- Eccentric reducers
- Equal tees
- Reducing tees
- End caps
This article is a summary of the mechanical properties
As an alternative to scanning down the list try the ‘find’ facility on your keyboard, using the ‘Ctrl’ and ‘F’ keys together. Type in the term you are looking for in the dialog box that then appears.
The data given is not intended to replace that shown in individual standards to which reference should always be made.
Steel grade |
Proof strength min MPA |
Tensile strength MPa |
Elongation A min % |
Resistance to intergranular corrosion |
Steel name |
Steel number |
Rp0.2 |
Rp1.0 |
Rm |
long |
trans |
Austenitic stainless steels |
X2CrNi18-9 |
1.4307 |
180 |
215 |
470/670 |
40 |
35 |
Yes |
X2CrNi19-11 |
1.4306 |
180 |
215 |
460/680 |
40 |
35 |
Yes |
X2CrNiN18-10 |
1.4311 |
270 |
305 |
550/760 |
35 |
30 |
Yes |
X5CrNi18-10 |
1.4301 |
195 |
230 |
500/700 |
40 |
35 |
Yes* |
X6CrNiTi18-10 |
1.4541 |
200 |
235 |
500/730 |
35 |
30 |
Yes |
X6CrNiNb18-10 |
1.4550 |
205 |
240 |
510/740 |
35 |
30 |
Yes |
X2CrNiMo18-14-3 |
1.4335 |
190 |
225 |
490/690 |
40 |
30 |
Yes |
X2CrNiMo17-12-2 |
1.4404 |
190 |
225 |
490/690 |
40 |
30 |
Yes |
X5CrNiMo17-12-2 |
1.4401 |
205 |
240 |
510/710 |
40 |
30 |
Yes* |
XCrNiMoTi17-12-2 |
1.4571 |
210 |
245 |
500/730 |
35 |
30 |
Yes |
X2CrNiMo17-12-3 |
1.4432 |
190 |
225 |
490/690 |
40 |
30 |
Yes |
X2CrNiMoN17-13-3 |
1.4429 |
295 |
330 |
580/800 |
35 |
30 |
Yes |
X3CrNiMo17-13-3 |
1.4436 |
205 |
240 |
510/710 |
40 |
30 |
Yes* |
X2CrNiMo18-14-3 |
1.4435 |
190 |
225 |
490/690 |
40 |
35 |
Yes |
X2CrNiMoN17-13-5 |
1.4439 |
285 |
315 |
580/800 |
35 |
30 |
Yes |
X2CrNiMo18-15-4 |
1.4438 |
220 |
250 |
490/690 |
35 |
30 |
Yes |
X1CrMoCu31-27-4 |
1.4563 |
215 |
245 |
500/750 |
40 |
35 |
Yes |
X1CrNiMoCu25-20-5 |
1.4539 |
220 |
250 |
520/720 |
35 |
30 |
Yes |
X1CrNiMoCuN20-18-7 |
1.4547 |
300 |
340 |
650/850 |
35 |
30 |
Yes |
X1NiCrMoCuN25-20-7 |
1.4529 |
300 |
340 |
600/800 |
40 |
40 |
yes |
Austenitic ferritic steels |
X2CrNiMoN22-5-3 |
1.4462 |
450 |
|
700/920 |
25 |
20 |
Yes |
X2CrNiN23-4 |
1.4362 |
400 |
|
600/820 |
25 |
25 |
Yes |
X2CrNiMoN25-7-4 |
1.4410 |
550 |
|
800/1000 |
20 |
20 |
Yes |
X2CrNiMoCuWN25-7-4 |
1.4501 |
550 |
|
800/1000 |
20 |
20 |
Yes |
X2CrNiMoCuN25-6-3 |
1.4507 |
500 |
|
700/900 |
20 |
20 |
Yes |
* Normally not fulfilled in the sensitised or as-welded condition
BS EN 10253-4 has additional impact values at room temperature and – 196 deg C for austenitic stainless steels and at room temperature and -40 deg C for austenitic-ferritic stainless steels.