6a. Tolerances to ISO 9445 for cold rolled narrow and wide strip, plate/sheet and cut lengths

General

This standard is designed to bring together tolerances for cold rolled narrow and wide strip. It has officially superseded EN 10258 and EN 10259 although of course customers and suppliers are entitled to continue to use these standards. In most respects the tolerances from these standards are identical to the ones in this new ISO standard. The major differences are:

  1. Additional table for wide strip is included which is based on Japanese practice.
  2. Slightly different edge camber tolerances than in EN 10259 for wide strip.
  3. Provision for width tolerance on wide strip with mill edges.

Narrow strip is defined as having a rolled width of < 600mm and thickness < 3mm. This is the same definition as in EN 10258. This covers material slit from such products and cut lengths.

Wide strip is defined as having a rolled width of 600 – 2100 mm from 0.3-8.0mm thick. It therefore includes material slit from this product with actual width < 600mm and sheet/plate

The phrase “specified thickness” is preferred to “nominal thickness” in this ISO standard.

There is a view that the combination of all cold rolled products into one standard can be confusing. There are moves towards separating out narrow and wide products into two standards. This summary adopts this approach as for every tolerance type there are different values for narrow and wide products.

Narrow strip

Thickness tolerance

Tolerances on specified thickness for narrow cold rolled strip
Specified Thickness (t)
w < 125 125 < w < 250 250 < w < 600
Normal Fine (F) Precision(P) Normal Fine (F) Precision(P) Normal Fine (F) Precision(P)
0.05 < t < 0.10 ±0.10t ±0.06t ±0.04t ±0.12t ±0.10t ±0.08t ±0.15t ±0.10t ±0.08t
0.10 < t < 0.15 ± 0.010 ±0.008 ±0.006 ±0.015 ±0.012 ±0.008 ±0.020 ±0.015 ±0.010
0.15 < t < 0.20 ±0.015 ±0.010 ±0.008 ±0.020 ±0.012 ±0.010 ±0.025 ±0.015 ±0.012
0.20 < t < 0.25 ±0.015 ±0.012 ±0.008 ±0.020 ±0.015 ±0.010 ±0.025 ±0.020 ±0.012
0.25 < t < 0.30 ±0.017 ±0.012 ±0.009 ±0.025 ±0.015 ±0.012 ±0.030 ±0.020 ±0.015
0.30 < t < 0.40 ±0.020 ±0.015 ±0.010 ±0.025 ±0.020 ±0.012 ±0.030 ±0.025 ±0.015
0.40 < t < 0.50 ±0.025 ±0.020 ±0.012 ±0.030 ±0.020 ±0.015 ±0.035 ±0.025 ±0.018
0.50 < t < 0.60 ±0.030 ±0.020 ±0.014 ±0.030 ±0.025 ±0.015 ±0.040 ±0.030 ±0.020
0.60 < t < 0.80 ±0.030 ±0.025 ±0.015 ±0.035 ±0.030 ±0.018 ±0.040 ±0.035 ±0.025
0.80 < t < 1.00 ±0.030 ±0.025 ±0.018 ±0.040 ±0.030 ±0.020 ±0.050 ±0.035 ±0.025
1.00 < t < 1.20 ±0.035 ±0.030 ±0.020 ±0.045 ±0.035 ±0.025 ±0.050 ±0.040 ±0.030
1.20 < t < 1.50 ±0.040 ±0.030 ±0.020 ±0.050 ±0.035 ±0.025 ±0.060 ±0.045 ±0.030
1.50 < t < 2.00 ±0.050 ±0.035 ±0.025 ±0.060 ±0.040 ±0.030 ±0.070 ±0.050 ±0.035
2.00 < t < 2.50 ±0.050 ±0.035 ±0.025 ±0.070 ±0.045 ±0.030 ±0.080 ±0.060 ±0.040
2.50 < t < 3.00 ±0.060 ±0.045 ±0.030 ±0.070 ±0.050 ±0.035 ±0.090 ±0.070 ±0.045
  1. This table is identical to the table in EN 10258.
  2. By agreement the tolerances may alternatively be totally + or totally – or unevenly distributed. In any case the total tolerance shall be as in the table.
  3. For thicknesses below 0.05mm the values for the tolerances are to be agreed at the time of the enquiry and order.

Width tolerance

Tolerances on width for narrow cold rolled strip and cut lengths
Specified

Thickness (t)

Specified Width (w)
< 40 40 < w < 125 125 < w < 250 250 < w < 600
Normal Fine (F) Precision (P) Normal Fine (F) Precision (P) Normal Fine (F) Precision (P) Normal Fine (F) Precision (P)
 t < 0.25 +0.17/-0 +0.13/-0  +0.10/-0 +0.20/-0 +0.15/-0 +0.12/-0 +0.25/-0 +0.20/-0 +0.15/-0 +0.50/-0 +0.50/-0 +0.40/-0
0.25 < t < 0.50 +0.20/-0 +0.15/-0 +0.12/-0 +0.25/-0 +0.20/-0 +0.15/-0 +0.30/-0 +0.22/-0 +0.17/-0 +0.60/-0 +0.50/0 +0.40/-0
0.50 < t < 1.00 +0.25/-0 +0.20/-0 +0.15/-0 +0.25/-0 +0.22/-0 +0.17/-0 +0.40/-0 +0.25/-0 +0.20/-0 +0.70/-0 +0.60/-0 +0.50/-0
1.00 < t < 1.50 +0.25/-0 +0.22/-0 +0.15/-0 +0.30/-0 +0.25/-0 +0.17/-0 +0.50/-0 +0.30/-0 +0.22/-0 +1.0/-0 +0.70/-0 +0.60/-0
1.50 < t < 2.50 +0.40/-0 +0.25/-0 +0.20/-0 +0.60/-0 +0.40/-0 +0.25/-0 +1.0/-0 +0.80/-0 +0.60/-0
2.50 < t < 3.00 +0.50/-0 +0.3/-0 +0.25/-0 +0.6/-0 +0.40/-0 +0.25/-0 +1.2/-0 +1.0/-0 +0.80/-0

 

  1. This table is identical to the one in EN 10258.
  2. By agreement, the tolerances may be equally ± or all negative. In both cases, the total range of the tolerances shall be as in the table.

Length tolerance

 

Length tolerances for cut lengths from narrow strip
Specified length L Tolerances
Normal Special
< 2000 +3/-0 +1.5/-0
2000 < L < 4000 +5/-0 +2/-0
  1. This is identical to the table in EN 10258

Edge camber

 

Tolerances on edge camber for cold rolled narrow strip and cut lengths
Specified width w         Edge camber tolerances for measuring lengths
1000 2000 1000 2000
Normal Precision
  10 < w <   25 4 16 1.5 6
  25 < w <   40 3 12 1.25 5
  40 < w < 125 2 8 1.0 4
125 < w < 600 1.5 6 0.75 3
  1. This table is identical to the one in EN 10258.
  2. If applicable, both measuring lengths shall be used.
  3. These tolerances do not apply to the work hardened condition. Any requirement for this material shall be agreed at the time of enquiry and order.

Out of squareness

The out of squareness tolerance for cut lengths from narrow strip > 250mm shall not exceed 0.5% of the actual width of the product.

For widths < 250mm the tolerances shall be agreed at the time of enquiry and order.

These requirements are identical to those in EN 10258.

Flatness

The flatness tolerance for cut lengths from narrow strip shall not exceed 10mm for normal cases and 7mm where a special tolerance is required.

This does not apply to material in the work hardened condition which must be agreed at the time of the enquiry and order.

These requirements are identical to those in EN 10258.

Edge Waviness

For skin passed or stretch levelled narrow strip, the ratio of the wave height to wave length shall be a maximum of 0.03 for specified thicknesses < 1.00mm and a maximum of 0.02 for > 1.00mm.

These requirements are identical to those in EN 10258.

———————————————————————————————————————————————————

Wide strip

Thickness tolerance

The standard allows for two methods for defining thicknesses tolerance:

Method A – identical to EN 10259. Thickness is measured at any point located more than 20mm from the edge for slit edges and 30mm for mill edges.

Method B – Thickness is measured at any point located more than 15mm from the edge for slit edges and 25mm for mill edges. This is similar to Japanese standards.

 

Tolerances on specified thickness for cold rolled wide strip Method A
Specified thickness (t)  Normal tolerances for a nominal width w of  Special tolerances (S) for a nominal width w of
w<1000 1000<w<1300</w 1300<w<2100</w w<1000 1000<w<1300</w 1300<w<2100</w
            t < 0.30 ±0.030            —            — ±0.020           —            —
0.30 < t < 0.50 ±0.04 ±0.04            — ±0.025 ±0.030            —
0.50 < t < 0.60 ±0.045 ±0.05            — ±0.030 ±0.035            —
0.60 < t < 0.80 ±0.05 ±0.05            — ±0.035 ±0.040            —
0.80 < t < 1.00 ±0.055 ±0.06 ±0.06 ±0.040 ±0.045 ±0.050
1.00 < t < 1.20 ±0.06 ±0.07 ±0.07 ±0.045 ±0.045 ±0.050
1.20 < t < 1.50 ±0.07 ±0.08 ±0.08 ±0.050 ±0.055 ±0.060
1.50 < t < 2.00 ±0.08 ±0.09 ±0.10 ±0.055 ±0.060 ±0.070
2.00 < t < 2.50 ±0.09 ±0.10 ±0.11      —           —            —
2.50 < t < 3.00 ±0.11 ±0.12 ±0.12      —           —            —
3.00 < t < 4.00 ±0.13 ±0.14 ±0.14      —           —            —
4.00 < t < 5.00 ±0.14 ±0.15 ±0.15      —           —            —
5.00 < t < 6.50 ±0.15 ±0.15 ±0.16      —           —            —
6.50 < t < 8.00 ±0.16 ±0.17 ±0.17
  1. This table is similar to that in EN 10259 except that there is an extra line for 6.50 < t < 8.00.
  2. Also there are some differences in the number of decimal places for Special tolerances.
  3. Thickness is measured at any point located more than 20mm from the edge for slit edges and 30mm for mill edges – defined as Method A.
  4. For strip and cut lengths < 30mm wide the thickness shall be measured at the centre of the strip.
Tolerances on specified thickness for cold rolled wide strip Method B
Specified thickness (t)  Normal tolerances for a nominal width w of  Special tolerances (S) for a nominal width w of
w<1000 1000<w<1300</w 1300<w<2100</w w<1000 1000<w<1300</w 1300<w<2100</w
            t < 0.30 ±0.030            —            — ±0.030           —            —
0.30 < t < 0.50 ±0.04 ±0.04            — ±0.030 ±0.035            —
0.50 < t < 0.60 ±0.045 ±0.05            — ±0.035 ±0.035            —
0.60 < t < 0.80 ±0.05 ±0.05            — ±0.040 ±0.040            —
0.80 < t < 1.00 ±0.055 ±0.06 ±0.07 ±0.040 ±0.050 ±0.050
1.00 < t < 1.20 ±0.06 ±0.07 ±0.08 ±0.050 ±0.055 ±0.060
1.20 < t < 1.50 ±0.08 ±0.08 ±0.10 ±0.055 ±0.060 ±0.060
1.50 < t < 2.00 ±0.08 ±0.09 ±0.11 ±0.065 ±0.070 ±0.080
2.00 < t < 2.50 ±0.09 ±0.11 ±0.13      —           —            —
2.50 < t < 3.00 ±0.11 ±0.13 ±0.15      —           —            —
3.00 < t < 4.00 ±0.14 ±0.15 ±0.16      —           —            —
4.00 < t < 5.00 ±0.15 ±0.17 ±0.19      —           —            —
5.00 < t < 6.00 ±0.17 ±0.20 ±0.23      —           —            —
6.00 < t < 8.00 ±0.17 ±0.22 ±0.25
  1. Thickness is measured at any point located more than 15mm from the edge for slit edges and 25mm for mill edges – defined as Method B.
  2. For strip and cut lengths < 30mm wide the thickness shall be measured at the centre of the strip.
  3. Note the difference in the last two thickness bands compared to Method A.

 Width tolerance

Provision is made in this standard for width tolerances for mill edges.

For wide strip and sheet/plate cut from wide strip with mill edges < 1000mm, the tolerance is +25/-0mm.

For wider material the tolerance is +30/-0mm.

For wide strip with slit edges the tolerances are as in the table below:

 

Tolerances on wide cold rolled strip and sheet/plate cut from wide strip
Specified thickness (t)  Normal tolerances  for a specfied width w of Special tolerances (S)1) for a nominal width w of
w<125 125<w<250</w 250<w<600</w 600<w<1000</w 1000<w<2100</w w<125 125<w<250</w 250<w<600</w
t < 1.00 +0.5/-0 +0.5/-0 +0.7/-0 +1.5/-0 +2.0/-0 +0.3/-0 +0.3/-0 +0.6/-0
1.00 < t < 1.50 +0.7/-0 +0.7/-0 +1.0/-0 +1.5/-0 +2.0/-0 +0.4/-0 +0.5/-0 +0.7/-0
1.50 < t < 2.50 +1.0/-0 +1.0/-0 +1.2/-0 +2.0/-0 +2.5/-0 +0.6/-0 +0.7/-0 +0.9/-0
2.50 < t < 3.50 +1.2/-0 +1.2/-0 +1.5/-0 +3.0/-0 +3.0/-0 +0.8/-0 +0.9/-0 +1.0/-0
3.50 < t < 8.00 +2.0/-0 +2.0/-0 +1.2/-0 +4.0/-0 +4.0/-0      —       —      —
  1. By special agreement, products can be supplied with permissible undersizes on the nominal width. In this case, the values in this table apply as the oversize plus undersize range. E.g. 1.20 mm thick, 700 mm wide could be ordered to +1.0/-0.5mm by agreement.
  2. For material with edges re-cut by shearing, the tolerances on width may by agreement be increased to 5mm
  3. This table is similar to that in EN 10259 except that the highest nominal thickness is now 8.00mm.

Length tolerance

Length tolerances also have both ‘normal’ and ‘special’ tolerance ranges. ‘Special’ tolerance should be specifically requested. Each range is proportional to the length of the sheet or cut length, with a minimum tolerance at 2000mm length. Unlike the old standards, these tolerances apply for any length that can be supplied, and across the whole thickness range.

 

Nominal Length L Tolerances
Normal Special (S)
2000 +5/-0 +3/-0
2000 < L +0.0025 x L/-0 +0.0015 x L/-0
  1. This is identical to that in EN 10259

 Edge camber 

Tolerances on edge camber for wide strip and plate/sheet from wide strip
Specified width (w) Edge camber tolerances for measuring                                                          lengths
1000 2000
  10 < w <     40 2.5 10
  40 < w <   125 2 8
125 < w <   600 1.5 6
600 < w < 2100 1 4
  1. If applicable both measuring lengths shall be used.
  2. This table is the same as that in EN 10259 for widths from 40mm upwards. Two width bands in EN 10259 have been combined in this standard into the 10-40mm band and new values specified.

Out of Squareness

As in EN 10259 there are two ways to specify out of squareness and the values are identical to this standard.

Out of squareness is defined in Fig 2 below:

 

 

OR

Option 2 – shall not exceed the values in the table:

All dimensions in mm

Length L of sheet plate or cut length                              Maximum difference in diagonal lengths                                              
< 3000 6
3000 < L < 6000 10
> 6000 15

Ordered format

When ordering an agreement may be made that the ordered format (i.e. width and length) be contained in every piece supplied. In this case, the tolerances on width, length, edge camber and out of squareness shall be agreed at the time of the enquiry and order.

Flatness tolerance

The flatness tolerance of of strip, sheet/plate and cut length shall not exceed 10mm for normal cases and 7mm where a special tolerance (FS) is required for length < 3000mm and 12mm for normal cases and 8mm where a special tolerance (FS) is required for length > 3000mm.

This is identical to the requirements of EN 10259.

These requirements do not apply to work hardened material or condition 2D.

The flatness can be measured in the following ways:

a) For maximum deviation from a flat horizontal surface, with the product lying under its own mas on a flat surface, the maximum deviation from flatness in the maximum distance between the lower surface of the product and the flat horizontal surface.

b) To measure the flatness, the product shall be laid on an approximately flat surface. Deviation with respect to flatness shall be taken as the greatest distance between the product and a straight edge placed upon it. The straight edge should be either 1000 or 2000mm long. It may be placed on the product at any position and in any direction. Only the position of the points of contact of product and straight edge shall be taken into account.

Unless otherwise agreed, the choice of measurement methid is left to the manufacturer.

Edge waviness

For strip, the waviness of the edges, i.e. the ratio of wave height (h) to wave length (l) shall be max 0.03 for all thicknesses.

This requirement does not apply to work hardened material or condition 2D.