BS EN 10269 is the material standard for stainless and heat-resisting steels, a selection of low alloy steels and some nickel alloys for fasteners. The elevated and sub-zero temperature mechanical properties shown in this article include 0.2% proof and tensile strengths and impact (charpy) strength in the finally heat treated condition. The final heat treatment conditions for each grade are also tabulated.
As an alternative to scanning down the list try the ‘find’ facility on your keyboard, using the ‘Ctrl’ and ‘F’ keys together. Type in the term you are looking for in the dialog box that then appears.
The data given is not intended to replace that shown in individual standards to which reference should always be made.
Both 0.2% proof and tensile strengths are shown in the standard. These are shown below in separate tables.
Proof strengths
Designation | Condition | Max dia. mm | Minimum proof strength Rp0.2 N/mm2 at a temperature of (C) | |||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
Steel name | Steel number | 50 | 100 | 150 | 200 | 250 | 300 | 350 | 400 | 450 | 500 | 550 | 600 | 650 | ||
Steels for quenching and tempering | ||||||||||||||||
X22CrMoV12-1 | 1.4923 | QT1 | 160 | 585 | 560 | 545 | 530 | 505 | 480 | 450 | 420 | 380 | 335 | 280 | – | – |
QT2 | 160 | 681 | 650 | 625 | 600 | 575 | 550 | 518 | 485 | 440 | 390 | 330 | – | – | ||
X12CrNiMoV12-3 | 1.4938 | QT | 160 | 730 | 680 | 668 | 655 | 653 | 650 | 630 | 610 | 560 | 505 | 400 | – | – |
X19CrMoNbVN11-1 | 1.4913 | QT | 160 | 726 | 701 | 676 | 651 | 643 | 627 | 610 | 577 | 544 | 495 | 412 | 305 | – |
Austenitic Steels | ||||||||||||||||
X2CrNi18-9 | 1.4307 | AT | 160 | 164 | 145 | 130 | 118 | 108 | 100 | 94 | 89 | 85 | 81 | 80 | – | – |
X5CrNi18-10 | 1.4301 | AT | 160 | 177 | 155 | 140 | 127 | 118 | 110 | 104 | 98 | 95 | 92 | 90 | – | – |
X4CrNi18-12 | 1.4303 | AT | 160 | 177 | 155 | 140 | 127 | 118 | 110 | 104 | 98 | 95 | 92 | 90 | – | – |
X2CrNiMo17-12-2 | 1.4404 | AT | 160 | 187 | 165 | 150 | 137 | 127 | 119 | 113 | 108 | 103 | 100 | 98 | – | – |
X5CrNiMo17-12-2 | 1.4401 | AT | 160 | 191 | 175 | 158 | 145 | 135 | 127 | 120 | 115 | 112 | 110 | 108 | – | – |
X2CrNiMoN17-13-3 | 1.4429 | AT | 160 | 256 | 215 | 195 | 175 | 165 | 155 | 150 | 145 | 140 | 138 | 136 | – | – |
X6CrNi18-10 | 1.4948 | AT | 160 | 174 | 157 | 142 | 127 | 117 | 108 | 103 | 98 | 93 | 88 | 83 | 78 | – |
X10CrNiMoMnNbVB15-10-1 | 1.4982 | AT + WW | 100 | 490 | 463 | 446 | 434 | 423 | 413 | 405 | 396 | 391 | 386 | 378 | 365 | 346 |
X3CrNiMoBN17-13-3 | 1.4910 | AT | 160 | 239 | 205 | 187 | 170 | 159 | 148 | 141 | 134 | 130 | 127 | 124 | 121 | – |
X6CrNiMoB17-12-2 | 1.4919 | AT | 160 | 194 | 177 | 162 | 147 | 137 | 127 | 122 | 118 | 112 | 108 | 103 | 98 | – |
X6CrNiTiB18-10 | 1.4941 | AT | 160 | 183 | 162 | 152 | 142 | 137 | 132 | 127 | 123 | 118 | 113 | 108 | 103 | – |
X6NiCrTiMoVB25-15-2 | 1.4980 | AT + P | 160 | 592 | 580 | 570 | 560 | 550 | 540 | 530 | 520 | 510 | 490 | 460 | 430 | 380 |
X7CrNiMoBNb16-16 | 1.4986 | WW +P | 100 | 489 | 470 | 451 | 432 | 412 | 393 | 372 | 353 | 334 | 314 | 284 | 255 | 206 |
Tensile strengths
Designation | Condition | Max dia. mm | Minimum tensile strength Rm N/mm2 at a temperature of ( C) | |||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
Steel name | Steel number | 50 | 100 | 150 | 200 | 250 | 300 | 350 | 400 | 450 | 500 | 550 | 600 | 650 | ||
Austenitic steels | ||||||||||||||||
X2CrNi18-9 | 1.4307 | AT | 160 | 440 | 410 | 380 | 360 | 350 | 340 | 340 | 330 | – | – | – | – | – |
X5CrNi18-10 | 1.4301 | AT | 160 | 480 | 450 | 420 | 400 | 390 | 380 | 380 | 380 | 375 | 360 | 335 | 300 | – |
X4CrNi18-12 | 1.4303 | AT | 160 | 480 | 450 | 420 | 400 | 390 | 380 | 380 | 380 | 375 | 360 | 335 | 300 | – |
X2CrNiMo17-12-2 | 1.4404 | AT | 160 | 460 | 430 | 410 | 390 | 385 | 380 | 380 | 380 | 375 | 360 | 335 | – | – |
X5CrNiMo17-12-2 | 1.4401 | AT | 160 | 480 | 460 | 440 | 420 | 415 | 410 | 410 | 410 | 405 | 390 | 375 | 350 | – |
X2CrNiMoN17-13-3 | 1.4429 | AT | 160 | 550 | 520 | 490 | 460 | 450 | 440 | 435 | 435 | 435 | 430 | 410 | 380 | – |
X6CrNi18-10 | 1.4948 | AT | 160 | 480 | 450 | 420 | 400 | 390 | 380 | 380 | 380 | 375 | 360 | 335 | 300 | – |
X10CrNiMoMnNbVB15-10-1 | 1.4982 | AT + WW | 160 | 610 | 565 | 530 | 505 | 490 | 475 | 465 | 460 | 450 | 440 | 430 | 410 | 390 |
X3CrNiMoBN17-13-3 | 1.4910 | AT | 160 | 550 | 520 | 490 | 460 | 450 | 440 | 435 | 435 | 435 | 430 | 410 | 380 | – |
X6CrNiMoB17-12-2 | 1.4919 | AT | 160 | 490 | 460 | 440 | 420 | 415 | 410 | 410 | 410 | 405 | 390 | 375 | 350 | – |
X6CrNiTiB18-10 | 1.4941 | AT | 160 | 490 | 460 | 440 | 420 | 415 | 410 | 410 | 410 | 405 | 390 | 375 | 350 | – |
X6NiCrTiMoVB25-15-2 | 1.4980 | AT +P | 160 | n.a. | n.a. | n.a. | n.a. | n.a. | n.a. | n.a. | 720 | 710 | 700 | 690 | 670 | – |
X7CrNiMoBNb16-16 | 1.4986 | WW +P | 100 | 635 | 615 | 590 | 570 | 550 | 530 | 505 | 485 | 460 | 440 | 420 | 395 | 375 |
Designation | Condition | Max dia. mm | Minimum impact energy J (ISO-V test pieces) at a temperature of ( C) | |||
---|---|---|---|---|---|---|
Steel name | Steel number | -270 | -196 | +20 | ||
Austenitic steels | ||||||
X2CrNi18-9 | 1.4307 | C700 | 35 | – | 50 | 80 |
X5CrNi18-10 | 1.4301 | AT | 160 | – | 60 | 100 |
C700 | 35 | – | 50 | 80 | ||
X4CrNi18-12 | 1.4303 | AT | 160 | – | 60 | 100 |
C700 | 35 | – | 50 | 80 | ||
X2CrNiMo17-12-2 | 1.4404 | C700 | 35 | – | 50 | 80 |
X5CrNiMo17-12-2 | 1.4401 | C700 | 35 | – | 50 | 80 |
X2CrNiMoN17-13-3 | 1.4429 | AT | 160 | 50 | 60 | 100 |
X6CrNi18-10 | 1.4948 | AT | 160 | – | 60 | 100 |
X3CrNiMoBN17-13-3 | 1.4910 | AT | 160 | 50 | 60 | 100 |
X6CrNiMoB17-12-2 | 1.4919 | AT | 160 | – | 60 | 100 |
X6CrNiTiB18-10 | 1.4941 | AT | 160 | – | 60 | 100 |
X6NiCrTiMoVB25-15-2 | 1.4980 | AT+ P | 160 | – | 40 | 50 |
Note
Cold worked condition C700 for austenitic grades represents a minimum tensile strength of 700 N/mm2
Steel number | H T Symbol | Quench/anneal (1) | Cooling (2) | Temper (3) |
---|---|---|---|---|
1.4923 | QT1 | 1020/1070 | a,o,w | 680/740 |
QT2 | 1020/1070 | a,o,w | 660/720 | |
1.4938 | QT | 1035/1062 | o | 600/670 |
1.4913 | QT | 1100/1130 | a,o | 670/720 |
1.4307, 1.4301, 1.4303, 1.4567 | AT | 1000/1100 | w,a | – |
1.4404, 1.4401, 1.4429, | AT | 1020/1120 | w,a | – |
1.4948 | AT | 1000/1080 | w,a | – |
1.4982 | AT + WW | 1030/1070+650/750 | w+a | – |
1.4910, 1.4919 | AT | 1020/1100 | w,a | – |
1.4941 | AT | 1070/1150 | w,a | – |
1.4980 | AT + P | 970/990 | o,w | 710/730 |
1.4986 | WW + P | WW at 750/850 | – | 750/800 |
Notes
(1) Quenching or solution annealing temperature C
(2) Type of cooling a – air ; o – oil ; w – water
(3) Tempering or precipitation treatment temperature C
AT – solution annealed QT – quenched and tempered P – precipitation hardened WW – warm worked