BS 3146-2 is the material standard for stainless steel and some nickel based alloy castings, to be made by the investment (or lost wax) process. Martensitic, precipitation hardening, austenitic austenitic-ferritic (duplex) grades are included. The chemical composition of the stainless steel and some nickel based alloys in the standard are listed.
Despite the advent of the European standards system, this BS is still current. See BSI Website. There is no EN standard which replaces it.
As an alternative to scanning down the list try the ‘find’ facility on your keyboard, using the ‘Ctrl’ and ‘F’ keys together. Type in the term you are looking for in the dialog box that then appears.
The data given is not intended to replace that shown in individual standards to which reference should always be made.
Grade | |||||||||
---|---|---|---|---|---|---|---|---|---|
Chemical composition (% by mass – max unless stated) | |||||||||
C | Si | Mn | P | S | Cr | Mo | Ni | Others | |
Martensitic Grades | |||||||||
ANC1- A | 0.15 | 0.2/1.2 | 0.2/1.0 | 0.035 | 0.035 | 11.5/13.5 | – | 1.0 | – |
ANC1- B | 0.12/0.2 | 0.2/1.2 | 0.2/1.0 | 0.035 | 0.035 | 11.5/13.5 | – | 1.0 | – |
ANC1- C | 0.2/0.3 | 0.2/1.2 | 0.2/1.0 | 0.035 | 0.035 | 11.5/13.5 | – | 1.0 | – |
ANC2 | 0.12/0.25 | 0.2/1.0 | 0.2/1.0 | 0.035 | 0.035 | 15.5/20.0 | – | 1.5/3.0 | – |
Austenitic Grades | |||||||||
ANC3 – A | 0.12 | 0.2/2.0 | 0.2/2.0 | 0.035 | 0.035 | 17.0/20.0 | – | 8.0/12.0 | – |
ANC3 – B | 0.12 | 0.2/2.0 | 0.2/2.0 | 0.035 | 0.035 | 17.0/20.0 | – | 8.5/12.0 | Nb 8xC/1.10 |
ANC4 – A | 0.08 | 0.2/1.5 | 0.2/2.0 | 0.035 | 0.035 | 18.0/20.0 | 3.0/4.0 | 11.0/14.0 | – |
ANC4 – B | 0.08 | 0.2/1.5 | 0.2/2.0 | 0.035 | 0.035 | 17.0/20.0 | 2.0/3.0 | 10.0 min | – |
ANC4 – C | 0.12 | 0.2/1.5 | 0.2/2.0 | 0.035 | 0.035 | 17.0/20.0 | 2.0/3.0 | 10.0 min | Nb 8xC/1.10 |
ANC5 – A | 0.5 | 0.2/3.0 | 0.20/2.0 | – | – | 22.0/27.0 | – | 17.0/22.0 | – |
ANC5 – B | 0.5 | 0.2/3.0 | – | – | 15.0/25.0 | – | 36.0/46.0 | – | – |
ANC5- C | 0.75 | 0.2/3.0 | 0.2/2.0 | – | – | 10.0/20.0 | – | 55.0/65.0 | – |
ANC6 – A | 0.15/0.3 | 0.75/2.0 | 0.2/1.0 | 0.035 | 0.035 | 20.0/25.0 | – | 10.0/15.0 | – |
ANC6 – B | 0.15/0.3 | 0.75/2.0 | 0.2/1.0 | 0.035 | 0.035 | 20.0/25.0 | – | 10.0/15.0 | W 2.5/3.5 |
ANC6 – C | 0.05/0.15 | 0.75/2.0 | 0.2/1.0 | 0.035 | 0.035 | 20.0/25.0 | – | 10.0/18.0 | W 2.5/3.5 |
Precipitation Hardening Grades | |||||||||
ANC20 A | 0.07 | 0.2/2.0 | 0.2/1.0 | 0.025 | 0.025 | 12.5/15.5 | 0.5/2.5 | 3.0/6.0 | Cu 1.0/3.5 Nb 0.5 |
ANC20 B | 0.07 | 0.2/2.0 | 0.2/1.0 | 0.025 | 0.025 | 12.5/15.5 | 0.5/2.5 | 3.0/6.0 | Cu 1.0/3.5 Nb 0.5 |
Duplex Grades | |||||||||
ANC21 | 0.05 | 0.75 | 0.75 | 0.050 | 0.050 | 25.0/27.0 | 1.75/2.25 | 4.75/6.00 | Cu 2.75/3.25 N 0.10 |
Note
For grades ANC1, ANC3 and ANC4, where specified, the sulphur (S) level may be as high as 0.3% where free machining properties are required.