As an alternative to scanning down the list try the ‘find’ facility on your keyboard, using the ‘Ctrl’ and ‘F’ keys together. Type in the term you are looking for in the dialog box that then appears.
The data given is not intended to replace that shown in individual standards to which reference should always be made.
BS EN 10028-7 was originally published in 2000. The second, current version, BS EN 10028-7:2007, has superseded BS EN 10028-7:2000, which was withdrawn by BSi on 31st January 2008.
The tables shown here only have the 2005 composition ranges.
The grades are taken mostly from BS EN 10088-2 with some grades from creep resisting standard BS EN 10302. The distinction between standard and special grades in BS EN 10088-2 is not followed through into this standard. The following tables preserve the listing in the standard which is not in grade number order.
Designation | Chemical composition % by mass max unless stated | ||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|
Steel name | Steel number | C | Si | Mn | P | S | N | Cr | Mo | Ni | Others |
Ferritic stainless steels | |||||||||||
X2CrNi12 | 1.4003 | 0.030 | 1.00 | 1.50 | 0.040 | 0.015 | 0.030 | 10.5/12.5 | – | 0.30/1.00 | – |
X6CrNiTi12 | 1.4516 | 0.08 | 0.70 | 1.50 | 0.040 | 0.015 | – | 10.5/12.5 | – | 0.50/1.50 | Ti: 0.05/0.35 |
X2CrTi17 | 1.4520 | 0.025 | 0.50 | 0.50 | 0.040 | 0.015 | 0.015 | 16.0/18.0 | – | – | Ti: 0.30/0.60 |
X3CrTi17 | 1.4510 | 0.05 | 1.00 | 1.00 | 0.040 | 0.015 | – | 16.0/18.0 | – | – | Ti: 4(C+N)+0.15/0.80 |
X2CrMoTi17-1 | 1.4513 | 0.025 | 1.00 | 1.00 | 0.040 | 0.015 | 0.015 | 16.0/18.0 | 0.80/1.40 | – | Ti: 0.30/0.60 |
X2CrMoTi18-2 | 1.4521 | 0.025 | 1.00 | 1.00 | 0.040 | 0.015 | 0.030 | 17.0/20.0 | 1.80/2.50 | – | Ti: 4(C+N)+0.15/0.80 |
X6CrMoNb17-1 | 1.4526 | 0.08 | 1.00 | 1.00 | 0.040 | 0.015 | 0.040 | 16.0/18.0 | 0.80/1.40 | – | Nb:7(C+N)+0.10/1.00 |
X2CrTiNb18 | 1.4509 | 0.030 | 1.00 | 1.00 | 0.040 | 0.015 | – | 17.5/18.5 | – | – | Ti: 0.10/0.60 Nb: 3C+0.30/1.00 |
Martensitic stainless steels | |||||||||||
X3CrNiMo13-4 | 1.4313 | 0.05 | 0.70 | 1.50 | 0.040 | 0.015 | >0.020 | 12.0/14.0 | 0.30/0.70 | 3.5/4.5 | |
X4CrNiMo16-5-1 | 1.4418 | 0.06 | 0.70 | 1.50 | 0.040 | 0.015 | >0.020 | 15.0/17.0 | 0.80/1.50 | 4.0/6.0 | |
Austenitic stainless steels | |||||||||||
X2CrNiN18-7 | 1.4318 | 0.030 | 1.00 | 2.00 | 0.045 | 0.015 | 0.10/0.20 | 16.5/18.5 | – | 6.0/8.0 | – |
X2CrNi18-9 | 1.4307 | 0.030 | 1.00 | 2.00 | 0.045 | 0.015 | 0.11 | 17.5/19.5 | – | 8.0/10.5 | – |
X2CrNi19-11 | 1.4306 | 0.030 | 1.00 | 2.00 | 0.045 | 0.015 | 0.11 | 18.0/20.0 | – | 10.0/12.0 | – |
X5CrNiN19-9 | 1.4315 | 0.06 | 1.00 | 2.00 | 0.045 | 0.015 | 0.12/0.22 | 18.0/20.0 | – | 8.0/11.0 | – |
X2CrNiN18-10 | 1.4311 | 0.030 | 1.00 | 2.00 | 0.045 | 0.015 | 0.12/0.22 | 17.5/19.5 | – | 8.5/11.5 | – |
X5CrNi18-10 | 1.4301 | 0.07 | 1.00 | 2.00 | 0.045 | 0.015 | 0.11 | 17.5/19.5 | – | 8.0/10.5 | – |
X6CrNiTi18-10 | 1.4541 | 0.08 | 1.00 | 2.00 | 0.045 | 0.015 | – | 17.0/19.0 | – | 9.0/12.0 | Ti: 5C/0.70 |
X6CrNiNb18-10 | 1.4550 | 0.08 | 1.00 | 2.00 | 0.045 | 0.015 | – | 17.0/19.0 | – | 9.0/12.0 | Nb: 10xC/1.00 |
X1CrNi25-21 | 1.4335 | 0.020 | 0.25 | 2.00 | 0.025 | 0.010 | 0.11 | 24.0/26.0 | 0.20 | 20.0/22.0 | – |
X2CrNiMo17-12-2 | 1.4404 | 0.030 | 1.00 | 2.00 | 0.045 | 0.015 | 0.11 | 16.5/18.5 | 2.00/2.50 | 10.0/13.0 | – |
X2CrNiMoN17-11-2 | 1.4406 | 0.030 | 1.00 | 2.00 | 0.045 | 0.015 | 0.12/0.22 | 16.5/18.5 | 2.00/2.50 | 10.0/12.0 | – |
X5CrNiMo17-12-2 | 1.4401 | 0.07 | 1.00 | 2.00 | 0.045 | 0.015 | 0.11 | 16.5/18.5 | 2.00/2.50 | 10.0/13.0 | – |
X1CrNiMoN25-22-2 | 1.4466 | 0.020 | 0.70 | 2.00 | 0.025 | 0.010 | 0.10/0.16 | 24.0/26.0 | 2.00/2.50 | 21.0/23.0 | – |
X6CrNiMoTi17-12-2 | 1.4571 | 0.08 | 1.00 | 2.00 | 0.045 | 0.015 | – | 16.5/18.5 | 2.00/2.50 | 10.5/13.5 | Ti: 5C/0.70 |
X6CrNiMoNb17-12-2 | 1.4580 | 0.08 | 1.00 | 2.00 | 0.045 | 0.015 | – | 16.5/18.5 | 2.00/2.50 | 10.5/13.5 | Nb: 10xC/1.00 |
X2CrNiMo17-12-3 | 1.4432 | 0.030 | 1.00 | 2.00 | 0.045 | 0.015 | 0.11 | 16.5/18.5 | 2.50/3.00 | 10.5/13.0 | – |
X2CrNiMoN17-3-3 | 1.4429 | 0.030 | 1.00 | 2.00 | 0.045 | 0.015 | 0.12/0.22 | 16.5/18.5 | 2.50/3.00 | 11.0/14.0 | – |
X3CrNiMo17-13-3 | 1.4436 | 0.05 | 1.00 | 2.00 | 0.045 | 0.015 | 0.11 | 16.5/18.5 | 2.50/3.00 | 10.5/13.0 | – |
X2CrNiMo18-14-3 | 1.4435 | 0.030 | 1.00 | 2.00 | 0.045 | 0.015 | 0.11 | 17.0/19.0 | 2.50/3.00 | 12.5/15.0 | – |
X2CrNiMoN18-12-4 | 1.4434 | 0.030 | 1.00 | 2.00 | 0.045 | 0.015 | 0.10/0.20 | 16.5/19.5 | 3.0/4.0 | 10.5/14.0 | – |
X2CrNiMo18-15-4 | 1.4438 | 0.030 | 1.00 | 2.00 | 0.045 | 0.015 | 0.11 | 17.5/19.5 | 3.0/4.0 | 13.0/16.0 | – |
X2CrNiMoN17-13-5 | 1.4439 | 0.030 | 1.00 | 2.00 | 0.045 | 0.015 | 0.12/0.22 | 16.5/18.5 | 4.0/5.0 | 12.5/14.5 | – |
X1NiCrMo31-27-4 | 1.4563 | 0.020 | 0.70 | 2.00 | 0.030 | 0.010 | 0.11 | 26.0/28.0 | 3.0/4.0 | 30.0/32.0 | Cu: 0.70/1.50 |
X1NiCrMoCu25-20-5 | 1.4539 | 0.020 | 0.70 | 2.00 | 0.030 | 0.010 | 0.15 | 19.0/21.0 | 4.0/5.0 | 24.0/26.0 | Cu: 1.20/2.00 |
X1CrNiMoCuN25-25-5 | 1.4537 | 0.020 | 0.70 | 2.00 | 0.030 | 0.010 | 0.17/0.25 | 24.0/26.0 | 4.7/5.7 | 24.0/27.0 | Cu: 1.00/2.00 |
X1CrNiMoCuN20-18-7 | 1.4547 | 0.020 | 0.70 | 1.00 | 0.030 | 0.010 | 0.18/0.25 | 19.5/20.5 | 6.0/7.0 | 17.5/18.5 | Cu: 0.50/1.00 |
X1NiCrMoCuN25-20-7 | 1.4529 | 0.020 | 0.50 | 1.00 | 0.030 | 0.010 | 0.15/0.25 | 19.0/21.0 | 6.0/7.0 | 24.0/26.0 | Cu: 0.50/1.50 |
Austenitic creep resisting steels | |||||||||||
X3CrNiMoBN17-13-3 | 1.4910 | 0.4 | 0.75 | 2.00 | 0.035 | 0.015 | 0.10/0.18 | 16.0/18.0 | 2.00/3.00 | 12.0/14.0 | B:0.0015/0.0050 |
X6CrNiTiB18-10 | 1.4941 | 0.04/0.08 | 1.00 | 2.00 | 0.035 | 0.015 | – | 17.0/19.0 | – | 9.0/12.0 | Ti: 5xC/ 0.80
B:0.0015/0.0050 |
X6CrNi18-10 | 1.4948 | 0.04/0.08 | 1.00 | 2.00 | 0.035 | 0.015 | 0.10 | 17.0/19.0 | – | 8.0/11.0 | – |
X6CrNi23-13 | 1.4950 | 0.04/0.08 | 0.70 | 2.00 | 0.035 | 0.015 | 0.10 | 22.0/24.0 | – | 12.0/15.0 | – |
X6CrNi25.20 | 1.4951 | 0.04/0.08 | 0.70 | 2.00 | 0.035 | 0.015 | 0.10 | 24.0/26.0 | – | 19.0/22.0 | – |
X5NiCrAlTi31-20 | 1.4958 (+RA) | 0.03/0.08 | 0.70 | 1.50 | 0.015 | 0.010 | 0.030 | 19.0/22.0 | – | 30.0/32.5 | Cu: 0.50
Nb:0.10 Ti:0.20/0.50 Al:0.20/0.50 Al+Ti:0.70 Co: 0.50 Ni+Co: 30.0/32.5 |
X8NiCrAlTi32-21 | 1.4959 | 0.05/0.10 | 0.70 | 1.50 | 0.015 | 0.010 | 0.030 | 19.0/22.0 | – | 30.0/34.0 | Cu: 0.50
Ti: 0.20/0.65 Al:0.20/0.65 Co: 0.50 Ni+Co: 30.0/34.0 |
X8CrNiNb16-13 | 1.4961 | 0.04/0.10 | 0.30/
0.60 |
1.50 | 0.035 | 0.015 | – | 15.0/17.0 | – | 12.0/14.0 | Nb: 10xC/1.20 |
Austenitic-ferritic stainless steels | |||||||||||
X2CrNiN23-4 | 1.4362 | 0.030 | 1.00 | 2.00 | 0.035 | 0.015 | 0.05/0.20 | 22.0/24.0 | 0.10/0.60 | 3.5/5.5 | Cu 0.10/0.60 |
X2CrNiMoN12-5-3 | 1.4462 | 0.030 | 1.00 | 2.00 | 0.035 | 0.015 | 0.10/0.22 | 21.0/23.0 | 2.50/3.50 | 4.5/6.5 | – |
X2CrNiMoCuN25-6-3 | 1.4507 | 0.030 | 0.70 | 2.00 | 0.035 | 0.015 | 0.20/0.30 | 24.0/26.0 | 3.0/4.0 | 6.0/8.0 | Cu: 1.00/2.50 |
X2CrNiMoN25-7-4 | 1.4410 | 0.030 | 1.00 | 2.00 | 0.035 | 0.015 | 0.24/0.35 | 24.0/26.0 | 3.0/4.5 | 6.0/8.0 | – |
X2CrNiMoCuWN25-7-4 | 1.4501 | 0.030 | 1.00 | 1.00 | 0.035 | 0.015 | 0.20/0.30 | 24.0/26.0 | 3.0/4.0 | 6.0/8.0 | Cu: 0.50/1.00 W: 0.50/1.00 |
Element | Specified Limits on Cast Analysis (%) | Permissible tolerance on product analysis (%) | |
Carbon | < 0.030 | +0.005 | |
> 0.030 | < 0.10 | ±0.01 | |
Silicon | < 1.00 | ±0.05 | |
Manganese | < 1.00 | +0.03 | |
> 1.00 | < 2.00 | ±0.04 | |
Phosphorus | < 0.045 | +0.005 | |
Sulphur | < 0.015 | +0.003 | |
Nitrogen | < 0.35 | ±0.01 | |
Aluminium | < 0.65 | ±0.10 | |
Boron | > 0.0015 | < 0.0050 | ±0.0003 |
Chromium | > 10.5 | < 15.0 | ±0.15 |
> 15.0 | < 20.0 | ±0.20 | |
> 20.0 | < 28.0 | ±0.25 | |
Copper | < 1.00 | ±0.07 | |
> 1.00 | < 2.50 | ±0.10 | |
Molybdenum | <0.60 | ±0.03 | |
> 0.60 | < 1.75 | ±0.05 | |
> 1.75 | < 7.0 | ±0.10 | |
Niobium | < 1.20 | ±0.05 | |
Nickel | < 1.00 | ±0.03 | |
> 1.00 | < 5.0 | ±0.07 | |
> 5.0 | < 10.0 | ±0.10 | |
> 10.0 | < 20.0 | ±0.15 | |
> 20.0 | < 34.0 | ±0.20 | |
Cobalt | < 0.50 | ±0.05 | |
Titanium | < 0.80 | ±0.05 | |
Tungsten | < 2.50 | ±0.05 | |
Vanadium | < 0.20 | ±0.03 |